LOCTITE EA 9395
Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other
Main features
- 1,200 psi Lap Shear
- Thixotropic Application Control
- Ambient-Temperature Bonding Cure
Product Description
LOCTITE® EA 9395 AERO Epoxy Paste Adhesive is a two-component, ambient-temperature-curing epoxy adhesive with a thixotropic paste consistency and non-metallic filler. The mixed material is suitable for potting, filling and fairing applications and may be used with composite substrates, including applications where radar-absorbing material or structure considerations are important. After a five-day cure at 77°F/25°C, the adhesive provides a typical tensile lap shear strength of 4,300 psi (29.7 MPa) at 77°F/25°C and retains 1,200 psi (8.3 MPa) at 350°F/177°C on phosphoric-acid-anodized 2024-T3 AlClad aluminum under ASTM D1002 testing. The system uses a 100:17 mix ratio by weight and has a pot life of 95–100 minutes for a 450 g mass at 77°F/25°C.
Key features
- High-temperature strength retention: Retains a typical tensile lap shear strength of 1,200 psi (8.3 MPa) at 350°F/177°C under the documented ASTM D1002 test configuration.
- Thixotropic, non-metallic formulation: Supports paste application for potting, filling and fairing without the use of metallic filler.
- Ambient-temperature cure: Develops normal performance after five days at 77°F/25°C, with an alternative cure of one hour at 150°F/66°C.
Applications / Suitable for
- Potting applications
- Filling and fairing
- Composite-substrate assemblies
- Applications involving RAM/RAS considerations
TDS, SDS & Technical Documents
Technical Specifications
Physical Properties
General Properties
Additional Information
As-supplied / before-processing properties
Typical uncured component and mixed-material properties. Component identity, temperature and Brookfield test conditions are retained where supplied.
| Property | Value | Unit | Method / condition |
|---|---|---|---|
| Product form | Two-component thixotropic epoxy paste adhesive | — | As supplied |
| Filler type | Non-metallic | — | Formulation characteristic |
| Color, Part A | Light blue | — | Uncured |
| Color, Part B | Olive brown-black | — | Uncured |
| Color, mixed | Gray-blue | — | Immediately after mixing |
| Viscosity, Part A | 7,100 | poise | 77°F; Brookfield HBT, spindle 7 at 20 rpm |
| Viscosity, Part A | 710 | Pa·s | 25°C; Brookfield HBT, spindle 7 at 2.1 rad/s |
| Viscosity, Part B | 360 | poise | 77°F; Brookfield HBT, spindle 4 at 20 rpm |
| Viscosity, Part B | 36 | Pa·s | 25°C; Brookfield HBT, spindle 4 at 2.1 rad/s |
| Viscosity, mixed | 1,000–3,000 | poise | 77°F; Brookfield HBT, spindle 5 at 20 rpm |
| Viscosity, mixed | 100–300 | Pa·s | 25°C; Brookfield HBT, spindle 5 at 2.1 rad/s |
| Density, Part A | 1.42 | g/mL | Uncured component |
| Density, Part B | 1.00 | g/mL | Uncured component |
| Density, mixed | 1.31 | g/mL | Mixed adhesive |
| Mix ratio, Part A:Part B | 100:17 | parts by weight | Volume measurement is not recommended for structural applications unless precautions are taken to assure the correct ratio |
| Pot life | 95–100 | minutes | 450 g mass at 77°F/25°C; ASTM D2471, water bath |
| Handling strength | 24 | hours | At 77°F/25°C; full bond strength has not yet been attained |
| Standard cure schedule | 5 days | — | 77°F/25°C; normal performance |
| Alternative cure schedule | 1 hour | — | 150°F/66°C; normal performance |
| Shelf life, Part A | 1 | year | Stored below 40°F/4°C or below 77°F/25°C |
| Shelf life, Part B | 1 | year | Stored below 40°F/4°C or below 77°F/25°C |
After-processing / final-state properties
Typical cured adhesive and bonded-joint properties. Cure schedules, substrates, surface preparation, test temperatures and methods are retained because these conditions materially affect the results.
| Property | Value | Unit | Method / condition |
|---|---|---|---|
| Tensile lap shear strength | 2,300 / 15.8 | psi / MPa | Tested at −67°F/−55°C; ASTM D1002; cured 5 days at 77°F/25°C; 2024-T3 AlClad aluminum, phosphoric-acid anodized per ASTM D3933 |
| Tensile lap shear strength | 4,300 / 29.7 | psi / MPa | Tested at 77°F/25°C; ASTM D1002; documented aluminum preparation and cure |
| Tensile lap shear strength | 3,500 / 24.1 | psi / MPa | Tested at 180°F/82°C; ASTM D1002; documented aluminum preparation and cure |
| Tensile lap shear strength | 3,000 / 20.7 | psi / MPa | Tested at 250°F/121°C; ASTM D1002; documented aluminum preparation and cure |
| Tensile lap shear strength | 2,200 / 15.2 | psi / MPa | Tested at 300°F/149°C; ASTM D1002; documented aluminum preparation and cure |
| Tensile lap shear strength | 1,200 / 8.3 | psi / MPa | Tested at 350°F/177°C; ASTM D1002; documented aluminum preparation and cure |
| T-peel strength | 5–8 / 22–36 | lb/in / N/25 mm | 77°F/25°C; ASTM D1876; cured 5 days at 77°F/25°C; phosphoric-acid-anodized 2024-T3 AlClad aluminum |
| Bell peel strength | 15 / 67 | lb/in / N/25 mm | 77°F/25°C; ASTM D3167; cured 5 days at 77°F/25°C; phosphoric-acid-anodized 2024-T3 AlClad aluminum |
| Service temperature | Approximately 350 / 177 | °F / °C | Defined as the temperature at which the adhesive retains 1,000 psi/6.9 MPa by ASTM D1002 |
| Tensile strength | 8,070 / 55.6 | psi / MPa | 77°F/25°C; ASTM D638; 0.125 in/3.18 mm casting cured 5 days at 77°F/25°C |
| Tensile modulus | 717 / 4,940 | ksi / MPa | 77°F/25°C; ASTM D638; documented casting and cure |
| Elongation at break | 2.6 | % | 77°F/25°C; ASTM D638; documented casting and cure |
| Shore D hardness | 90 | Shore D | 77°F/25°C |
| Glass transition temperature, Tg | 163 / 73 | °F / °C | Tan delta by DMTA |
| Shear modulus, dry | 224 / 1,543 | ksi / MPa | 77°F/25°C |
| Compressive strength | 22,700 / 156.4 | psi / MPa | −67°F/−55°C; ASTM D695; cylindrical specimen 0.5 in/12.7 mm diameter × 1 in/25.4 mm |
| Compressive strength | 14,000 / 96.5 | psi / MPa | 75°F/25°C; ASTM D695; documented cylindrical specimen |
| Compressive strength | 10,100 / 69.6 | psi / MPa | 250°F/121°C; ASTM D695; documented cylindrical specimen |
| Compressive strength | 6,800 / 46.9 | psi / MPa | 350°F/177°C; ASTM D695; documented cylindrical specimen |
| Compressive modulus | 429 / 2,956 | ksi / MPa | 77°F/25°C; ASTM D695 |
| Dielectric constant | 4.22 | — | 0.1 kHz; ASTM D150 |
| Dielectric constant | 4.13 | — | 1.0 kHz; ASTM D150 |
| Dielectric constant | 3.97 | — | 10.0 kHz; ASTM D150 |
| Dissipation factor | 0.016 | — | 0.1 kHz; ASTM D150 |
| Dissipation factor | 0.021 | — | 1.0 kHz; ASTM D150 |
| Dissipation factor | 0.033 | — | 10.0 kHz; ASTM D150 |