LOCTITE EA 9360
Harmonization Code : 3506.91.90.99 | Prepared glues and other prepared adhesives, not elsewhere specified or included; products suitable for use as glues or adhesives, put up for retail sale as glues or adhesives, not exceeding a net weight of 1 kg ; Adhesives based on polymers of headings 3901 to 3913 or on rubber; Other ; Other
Main features
- Toughened Structural Epoxy Bonding
- 50-Minute Assembly Pot Life
- Room-Temperature Aircraft Bonding Cure
Product Description
LOCTITE® EA 9360 AERO is a two-component, toughened epoxy paste adhesive that cures at room temperature and combines high room-temperature peel strength with tensile lap shear performance at elevated temperatures. Its low-slump consistency supports controlled application, while the 50-minute pot life at 77°F (25°C), 200 g mass, provides time for mixing and assembly. The adhesive develops handling strength after 24 hours at 77°F (25°C) and reaches normal performance after a 5–7 day room-temperature cure. Accelerated curing may be used for small masses, including 1 hour at 180°F (82°C). It is also available in dual-cartridge packaging for two-component dispensing.
Key features
- High peel strength: Delivers a typical floating-roller peel strength of 68 lb/in (303 N/25 mm) after 7 days at 77°F (25°C) on prepared and primed 2024-T3 AlClad aluminum.
- Elevated-temperature bond performance: Retains typical tensile lap shear strength of 2,000 psi (13.8 MPa) at 225°F (107°C) on phosphoric-acid-anodized 2024-T3 bare aluminum.
- Room-temperature or accelerated cure: Reaches normal performance after 5–7 days at 77°F (25°C), with accelerated cures up to 200°F (93°C) available for small adhesive masses.
TDS, SDS & Technical Documents
Technical Specifications
General Properties
Mechanical Properties
Thermal Properties
Additional Information
As-supplied / before-processing properties
Typical uncured, mixing, working-time, storage and cure information for LOCTITE® EA 9360 AERO. Component and mixed-material values are identified separately.
| Property | Value | Unit | Method / condition |
|---|---|---|---|
| Product type | Two-component toughened epoxy paste adhesive | — | Requires mixing before application |
| Color — Part A | Off-white | — | Unmixed component |
| Color — Part B | Blue | — | Unmixed component |
| Viscosity — Part A | 3,000 | Poise | 77°F; Brookfield HBT, spindle 7 at 20 rpm |
| Viscosity — Part B | 1,700 | Poise | 77°F; Brookfield HBT, spindle 6 at 20 rpm |
| Viscosity — Mixed | 1,200 | Poise | 77°F; Brookfield HBT, spindle 5 at 20 rpm |
| Viscosity — Part A | 300 | Pa·s | 25°C; Brookfield HBT at 2.1 rad/s |
| Viscosity — Part B | 170 | Pa·s | 25°C; Brookfield HBT at 2.1 rad/s |
| Viscosity — Mixed | 120 | Pa·s | 25°C; Brookfield HBT at 2.1 rad/s |
| Density — Part A | 1.16 | g/mL | Unmixed component |
| Density — Part B | 1.00 | g/mL | Unmixed component |
| Density — Mixed | 1.14 | g/mL | Mixed adhesive |
| Mix ratio by weight — Part A:Part B | 100:43 | Parts by weight | Components must be mixed thoroughly |
| Mix ratio by volume — Part A:Part B | 2:1 | Parts by volume | Volume measurement is not recommended for structural applications unless precautions ensure the correct ratio |
| Pot life | 50 | minutes | 200 g mass at 77°F (25°C); ASTM D2471, water bath |
| Maximum recommended mixed quantity | 450 | g | Do not mix larger quantities because hazardous heat buildup and uncontrolled decomposition may occur |
| Handling strength | 24 | hours | At 77°F (25°C); full bond strength has not yet developed |
| Room-temperature cure | 5–7 | days | At 77°F (25°C) to achieve normal performance |
| Example accelerated cure | 1 hour at 180°F (82°C) | — | Complete cure; accelerated cures up to 200°F (93°C) are for small masses only |
| Shelf life — Part A and Part B | 1 | year | Stored below 40°F (4°C) |
| Shelf life — Part A and Part B | 6 | months | Stored below 77°F (25°C) |
| Shelf life — Part A and Part B | 6 | months | Stored below 90°F (32°C) |